Page 1 of 5

Journal for Studies in Management and Planning

Available at http://internationaljournalofresearch.org/index.php/JSMaP

e-ISSN: 2395-0463

Volume 01 Issue 04

May 2015

Available online: http://internationaljournalofresearch.org/ P a g e | 401

GGBS as a Sustainable Construction Material & Its

Comparison with Fly Ash and RHA

Sourabh

Lecturar, CE Deptt Gian Jyoti Group of Institutes

sourabhgoliyan27@gmail.com

Abstract –

Sustainable development is the need of 21st century

and in the construction industry concrete is the most

widely used construction material owing to well- known advantages such as low cost, general

availability and wide applicability. Cement is major

constituent material of the concrete which produced

by natural raw material like lime and silica. The

major problem associated with the production of

cement is the emission of carbon-di-oxide which is

responsible for global warming. As a result 2the

search for any such material, which can be used as

an alternative or as a supplementary for cement,

should lead to global which should meet the special

combinations of sustainable construction and lowest

possible environmental impact by using industrial

waste without compromising on its strength and

durability, which will result in decrease of cement

production thus reduction in emission in green

house gases, in addition to sustainable management

of the waste. Hence, the researchers are currently

focused on use of waste material having cementing

properties, which can be added in cement concrete

as partial replacement of cement. The commonly

used materials are Ground Granulated Blast Furnace

Slag (GGBS), Rice Husk Ash (RHA) and Fly Ash.

This present paper outlines the utility of Ground

granulated blast furnace Slag (GGBS) as a

replacement of ordinary Portland cement and its

comparison with Fly Ash and RHA.

Keywords: Ground granulated blast furnace Slag

(GGBS), Rice Husk Ash (RHA), Fly Ash, Ordinary

Portland Cement (OPC), Compressive strength

Introduction

Today in the 21st century the sustainable

development is mandatory to protect the

environment. As a part of construction industry we

have to find out alternatives of ordinary Portland

cement because cement industry contributes around

5% of manmade CO2. As manufacturing of cement

release around 900 kg CO2 per 1 tonne

manufacturing of cement [1]. The challenge in front

of civil engineering community is to provide a

sustainable construction material without

compromising on its strength and durability

properties which will result in decrease of cement

production and also help in solid waste

management. In search of sustainable construction

material researchers find some materials which have

chemical composition likewise cement and can be

used as partial replacement of cement in concrete

without affecting the properties of concrete. Some

commonly used materials are Ground Granulated

Blast Furnace Slag (GGBS), Fly ash and Rice husk

ash (RHA).

Ground Granulated Blast Furnace Slag (GGBS) is

made from a by-product of the production of iron in

a blast furnace where iron ore, limestone and coke

Page 2 of 5

Journal for Studies in Management and Planning

Available at http://internationaljournalofresearch.org/index.php/JSMaP

e-ISSN: 2395-0463

Volume 01 Issue 04

May 2015

Available online: http://internationaljournalofresearch.org/ P a g e | 402

are heated to about 1500°C. When these materials

melt in the blast furnace, two products are

produced—molten iron, and molten slag. The

molten slag is lighter and floats on the top of the

molten iron. The molten slag comprises mostly

silicates and alumina from the original iron ore,

combined with some oxides from the limestone.

The process of granulating the slag involves cooling

the molten slag through high-pressure water jets.

The granulated slag is further processed by drying

and then ground to a very fine powder, which is

GGBS cement. [2]. GGBS is specified for its many

technical advantages and as a means of reducing the

environmental impact of the production of Portland

cement. GGBS has the chemical composition much

similar to Portland cement that it why it can replace

cement to higher levels.

Fly ash is the fine residue produced from the

combustion of pulverized coal in electric and steam

generating plants. In India, thermal power plants are

the main source for producing electricity. The use

of small percentages of fly ash in a variety of civil

engineering works is being carried out mainly for

economical reasons. Fly ash, being available, at

negligible or no cost is taking place of cement, a

costly construction raw material with the aim - one,

to solve the problem of disposal of fly ash in

environment and two, to get some financial benefit.

The use of fly ash in concrete has increased in last

20 years considerably [3].

Rice husk ash (RHA) is produced by burning the

outer shell of the paddy that comes out as a waste

product during milling of rice. Since they are bulky

disposal of husk present an enormous problem.

Each ton of paddy produces about 200kg of husk

and this rice husk can be effectively converted

through controlled burning. At around 500oC a

valuable siliceous product that can enhance the

durability of concrete in the chemical composition

of rice husk ash is obtained.

This paper summaries the utility of Ground

Granulated Blast Furnace Slag GGBS as a

sustainable construction material by use of

experimental research work that carried on GGBS

and its comparison with Fly ash and Rice husk ash

in terms of physical and chemical properties and

comparison of strength at same replacement amount

[4].

Physical Properties of GGBS

The ground cement powder is near-white in colour

and is a hydraulic cement, i.e. it has the property of

setting and hardening through chemical reaction

with water.

Table 1 Physical Properties of GGBS [5]

Colour Off-white powder

Bulk density (loose) 1.0–1.1 tonnes/m3

Bulk density

(vibrated)

1.2–1.3 tonnes/m3

Relative density 2.85–2.95

Surface area 400–600 m2

/kg

Particle size <40 microns

Chemical Properties of GGBS

GGBS comprises mainly of CaO, SiO2, Al2O3,

MgO it contains less than 1% crystalline silica, and

contains less than 1 ppm water soluble chromium

IV. It has the same main chemical constituents as

ordinary Portland cement, but in different

proportions

Table 2 Comparison of chemical properties of

GGBS with OPC [5]

Chemical

Constituents

OPC (%) GGBS (%)

CaO 65 40

SiO2 20 35

Al2O3 5 10

MgO 2 8

Comparison of Physical Properties of GGBS

with Fly Ash and RHA

Page 3 of 5

Journal for Studies in Management and Planning

Available at http://internationaljournalofresearch.org/index.php/JSMaP

e-ISSN: 2395-0463

Volume 01 Issue 04

May 2015

Available online: http://internationaljournalofresearch.org/ P a g e | 403

Table 3 Comparison of physical properties of

GGBS with Fly Ash and RHA

Property GGBS Fly Ash

[6]

RHA [7]

Colour Off-white

powder

Whitish

Grey

Grey

Bulk

density

1.0–1.3

g/cm3

0.994

g/cm3

0.34-0.40

g/cm3

Relative

density

2.85–2.95 2.288 2.3

Surface

area

400–600

m2

/kg

340-360

m2

/kg

18-20 m2

/g

Particle

size

<40

microns

Average

28.9 %

retained on

45 micron

sieve

25 microns

– mean

Comparison of Physical Properties of GGBS

with Fly Ash and RHA

Table 4 Comparison of chemical properties of

GGBS with Fly Ash and RHA

Chemical

Constituents

GGBS

(%)

Fly Ash

(%) [8]

RHA

(%) [9]

CaO 40 0.37-

27.68

1.8

SiO2 35 27.88-

59.40

83.60

Al2O3 10 5.23-

33.99

3.05

MgO 8 0.42-8.75 1.28

Experimental Research

1. Effect of GGBS on Compressive Strength

of Concrete at various replacement levels

[10]

Concrete made with GGBS attains the same

28–day strength as concrete made with

ordinary Portland cement, for replacement

levels of GGBS up to 50%. Concrete made

with GGBS continues to gain strength over a

very long period, and the ultimate strength

of concrete made with GGBS is consistently

higher than concrete made with ordinary

Portland cement. It is not unusual for a

GGBS concrete to increase its 28–day

strength by a further 20% at 90 days. In

laboratory investigations, GGBS concrete

was shown to double its 28–day strength

after 10 to 12 years. Typical strengths of

M35 concrete made with various

percentages of GGBS are shown in the table

5

Table 5

2. Resistance to Sulphate Attack co GGBS

based Concrete [11]

Attack by sulphates in ground water is a

common form of concrete deterioration.

Sulphates react with tri-calcium aluminate

(C3A) and calcium hydroxide (Ca(OH)2) to

form an expansive compound called

secondary ettringite. The expansion of the

ettringite causes concrete cracking, allowing

ingress of more sulphates and producing an

acceleration of the deterioration.

Sulphate resisting Portland cements (SRPC),

with low C3A content, are much less

effective in combating sulphate attack than

GGBS. GGBS counters sulphate attack in

three ways:

 GGBS does not contain any C3A,

and its inclusion in concrete reduces

GGBS

%

7 Day 28 Day 56 Day

0 32 42 43

20 30 43 45

35 27 43 47

50 23 44 44