Page 1 of 9
European Journal of Business &
Social Sciences
Available at https://ejbss.org/
ISSN: 2235-767X
Volume 07 Issue 04
April 2019
Available online: https://ejbss.org/ P a g e | 1815
Processing and Mechanical & Thermal Properties of Mudar Fiber
Reinforced Epoxy Composite
C. Selva Rama Subramanian1 pg scholar PRIST University Thanjavur.
Dr.B. Selva Sundaram2
,M.E.,Ph.D.,Assistant professor Einstein College of Engineering Tirunelveli
Abstract- The present work deals with the processing and mechanical & Thermal properties of Mudar fiber
reinforced epoxy composite. The mudar fibers were aligned by randomly and were prepared in square plate shape.
The mechanical properties like tensile. Compression and flexural strength were tested by varying the wt% of fiber
like 15%.20%.30% and 40% both treated and untreated fiber
Key words; Mudar fiber, treated and untreated fiber, Noah, Mechanical properties tensile, compression & flexural
strength
I. INTRODUCTION
A composite is a structural material that is
widely used for light weight and high strength
applications. It is commonly used in aerospace,
automobile and defence vehicles. General fiber
reinforced composites are combined of fiber and
matrix. The important function of the fibers is take
the loads along their longitudinal directions.
Modern composite materials constitute a
significant proportion of the engineered materials
market ranging from everyday products to
sophisticated niche applications. While composites
have already proven their worth as weight-saving
materials, the current challenge is to make them cost
effective. The efforts to produce economically
attractive composite components have resulted in
several innovative manufacturing techniques
currently being used in the composites industry.
It is obvious, especially for composites, that
the improvement in manufacturing technology alone
is not enough to overcome the cost hurdle. It is
essential that there be an integrated effort in design,
material, process, tooling, quality assurance,
manufacturing, and even program management for
composites to become competitive with metals.
The composites industry has begun to
recognize that the commercial applications of
composites promise to offer much larger business
opportunities than the aerospace sector due to the
sheer size of transportation industry. Thus the shift of
composite applications from aircraft to other
commercial uses has become prominent in recent
years.
Increasingly enabled by the introduction of
newer polymer resin matrix materials and high
performance reinforcement fibers of glass, carbon
and aramid, the penetration of these advanced
materials has witnessed a steady expansion in uses
and volume.
Most commonly used matrix materials are
polymeric. In general the mechanical properties of
polymers are inadequate for many structural
purposes. In particular their strength and stiffness are
low compared to metals and ceramics. These
difficulties are overcome by reinforcing other
materials with polymers. Secondly the processing of
polymer matrix composites need not involve high
pressure and does not require high temperature. Also
equipments required for manufacturing polymer
matrix composites are simpler.
Composites are used because overall
properties of the composites are superior to those of
the individual components for example
polymer/ceramic. Composites have a greater
modulus than the polymer component but are not as
brittle as ceramics.
They included roof for housing application,
structural panels and unit beams were manufactured
out of soybean oil based resin and natural fibers
(flax, cellulose, pulp, recycled paper, chicken
Page 2 of 9
European Journal of Business &
Social Sciences
Available at https://ejbss.org/
ISSN: 2235-767X
Volume 07 Issue 04
April 2019
Available online: https://ejbss.org/ P a g e | 1816
eathers) using vacuum assisted resin transfer molding
(VARTM) technology. Natural fiber reinforcement
of 20–55 wt % fiber increased the flexural modulus
to 2–6 GPa. The same resin reinforced with woven
E-glass gave a flexural modulus of 17 GPa. [1]
Scanning electron microscopy revealed some
interaction between the polymer and keratin feather
fiber. Physical property testing and microscopy show
some interaction between the fiber and polymer
without the need for coupling agents or chemical
treatment of the fibers. The density of the composite
upon introduction of keratin feather fiber is not
increased, but reduced by 2%. [2]
Glass fiber hybrid composites. Two types of
specimens are prepared, one by mixing the Palmyra
and glass fiber and the other by sandwiching Palmyra
fiber between the glass fiber mats. Composite plates
are prepared for different Palmyra/glass fiber weight
ratio. The tensile, bending, shear and impact
properties of roof light resin, Palmyra/glass fiber
hybrid composites are studied. The mechanical
properties increased due to hybridization.[3]
Composite Materials in pipes and pressure vessels.
Specimens cut from pipes made from composite
materials were tested under internal pressure loadings
have been tested by using a series of ASTM
Standards test methods for mechanical properties.
Good agreement was achieved between the
experimental results and analytical results.[4]
An alternative raw material for fiber- reinforced composite (FRC) . It is found that there
are statistically significant differences in the bark and
seed fiber dimensions. The bark fibers are long, with
a thin wall relative to their diameter, and are
therefore lightweight. The seed and bark fibers are
very similar to hard- and soft-woods, in terms of
chemical compositions and fiber dimensions,
respectively. Analyses conducted in this study
showed that there is a significant variation in the
holocellulose contents of the fractions of Mudar. The
higher content of holocellulose for bark fiber
provides a mechanical property of Mudar fibers are
in the range of non wood plant fibers.[5]
Reviewed the most suitable and commonly
used biodegradable polymer matrices and NF
reinforcements in eco-composites and nano
composites, with special focus on PLA Poly (lactic
acid) based materials. They concluded that, these can
represent an effective solution to the waste disposal
problem of polymer based materials.[6]
They said that before using the natural fiber,
the Fiber should be washed with 10% NaOH solution
and rinsed in hot water to remove the cellulose from
fiber surface for getting better binding with polymer
matrix. [7] The mean tensile strength, mean tensile
modulus and flexural modulus of vakka fiber
composite are much higher than those of sisal and
banana composites and comparable to that of
bamboo composite. The dielectric strength of vakka
fiber composites increases with increase in volume
fraction of fiber in the composite which is rare
phenomenon not observed in many of the natural
fiber composites. [8]
They Explained the resin, hardner standards
and density, Mould preparation, Casting of slabs,
Curing and sample preparation. They conclude that
the compressive strength has been found to increase
with increase in fly ash particles. In SEM analysis it
has been found that fly-ash particles have been
uniformly segregated.[9] Fibers treated with 5%,
10% and 15% NaOH and the effect of alkali
treatments on the fiber properties were explored. It is
concluded that 5% alkali treatment to the fibers
favored better mechanical properties to the Borassus
fruit fibers than the raw, 10% and 15% alkali treated
fibers. Hence the 5% NaOH treated Borassus fruit
fibers could be used as reinforcement in the
composites for structural applications.[10]
The results revealed that reinforcement of
epoxy with treated kenaf fibers increased the flexural
strength of the composite by about 36%, The
untreated fibers introduced 20% improvement. The
maximum strength of epoxy is about 225–250 MPa.
The treated kenaf fibers highly improved the flexural
strength of the epoxy composite which reached about
300–350 Mpa. [11] The simple hand lay-up
Page 3 of 9
European Journal of Business &
Social Sciences
Available at https://ejbss.org/
ISSN: 2235-767X
Volume 07 Issue 04
April 2019
Available online: https://ejbss.org/ P a g e | 1817
technique to prepare the composite specimen of
Snake grass in to polyester with various fiber length
(10,30,60,90,120,150 mm) and volume fractions (Vf)
like 10%, 15%, 20%, 25% and 30% respectively. The
maximum tensile strength and modulus of the
chopped fiber isophthallic polyester composite is
achieved at 25% Vf for the 30 mm fiber length.[12]
The work includes the Analysis of Palmyra
Fiber Reinforced Epoxy Composites using FEA with
various fiber volume fractions and these results were
validated with the experimental result. The
experimental results were compared with the
analytical result and error percentage was
determined. The error % is higher in untreated fiber
than 5% NAOH treated fiber. [13]
II. EXPERIMENTAL PROCEDURE
2.1 Extraction of fibers
The mudar fibers were extracted from dried
barks of CG plant. The CG plant is a shrub growing
up to 4 m height. These plants mostly grow in dry
areas. The fiber can be obtained from both seed and
bark. The seed fiber can be extracted by drying the
seeds in sunlight for two days and the seeds are
opened out, the fiber will be with bunch of seeds, the
seeds have to be removed to obtained seed fiber. The
barks are pealed out from CG plant and dipped in
water for 2 weeks and skin was separated. The fiber
is extracted manually from bark and the extracted
fiber is allowed to dry in room temperature for 7
days. The length of extracted fiber varies from 50mm
to 80mm this is because of presents of notches. The
seed fibers are easier to extract and it is very soft in
nature. The bark fiber has better mechanical
properties than seed fiber. The fiber for this research
was collected from plants in southern part of India.
2.2 Fibers alkaline treatment
The extracted mudar fibers have
holocellulose content present on the surface of fiber.
The NaOH treatment removes little amount of
cellulose from surface of fiber and removes the firing
particles and dirt. Mudar fibers were treated with 5%
sodium hydroxide solution at 300C, by dipping in the
alkali solution for 1h. [10] The fibers were then
washed with tap water repeatedly, neutralized with
dilute acetic acid, again washed with distilled water,
and dried in sun light for a period of 24 h.
2.3 Mould Preparation
The mould was prepared for
the size of 280x280x3mm3
and
280x55x3 mm3
. Figure 2.1 shows the
mould for the size of 280x280x3 mm3
.
The mould is made with a base plate of
10mm thickness and 3mm stripes are
bolted all around with distance
of280mm.
Figure 2.1 Mould for the size of
280x280x3mm3
2.4 Specimen preparation
Area of epoxy = 28x5.5x0.3=46.2cm3
Wight of epoxy=46.2cm3 x
1.1 g/cm3 =50.82g
Ω 50g